Re: lead loading

that's useful.. but what is the difference between lead solder sticks and lead, for the bit after the tinning of the surface.
It gets less sustainable if I can't use what is hanging around!


This has cross posted with Bob's - so answers some bits, thanks.

Re: lead loading

Wiping metal is not lead; it is 30% tin or somesuch which gives prolonged pastiness. And is expensive, unless like me your father was a plumber and you have inherited a stash.

Why struggle with panel distortion and sniff acid and lead fumes and absorb lead and contaminate workshop with lead dust and filings? Also risk of explosions due damp containers, burns due solder getting behind rings etc etc. Every trace of rust has to be removed for complete tinning, not just killed.

Cars are going to be molly coddled anyway. The door interiors, window seals, etc are not made for prolonged outdoor life.

The best feature of wiping metal is that it has no shelf life.

Location: Auckland, NZ

Email  
Re: lead loading

The guy doing my 65 body wouldn't dream of using lead, reckoning appropriate modern fillers far superior.

Location: Horley

Email  
Re: lead loading

Quote: JonE
that's useful.. but what is the difference between lead solder sticks and lead, for the bit after the tinning of the surface.
It gets less sustainable if I can't use what is hanging around!


This has cross posted with Bob's - so answers some bits, thanks.


Plumbers solder is usually 30% tin, 70% lead which is suitable for forming wiped joints in pipework
Tinmans solder is 70% tin, 30% lead which freezes more quickly to allow assembly.
I don't know the proportions for body filling but unless you're looking at very small imperfections I would practice long and hard before you set about your cherished car body.
Experts make it look easy, which it is when you know how. It's that "know how" which is the difficult bit!

Location: Ripon

Re: lead loading

Furthermore the acid flux vapouriese and condenses on everything in the workshop so all tools, the lathe, drill press etc all go rusty. Most everyday solder is/was 50/50.
Where rust holes will remain but will bridge, and a thickness can be applied, lead may be convenient. On "moderns" I have filled just below windows where the contour can be duplicated but raised. Can cover larger holes on either side with metal from tin cans.

Location: Auckland, NZ

Email  
Re: lead loading

Bob the Bodger writes again! Cheers, Bill in Oz

Location: Euroa,Victoria

Email  
Re: lead loading

To be serious, before any more newcomers are misled, the "cures" as suggested by Bob should not be attempted. Even lightly-rusted steel or lightly-corroded aluminium cannot be properly cured by covering with plastic-type body-bog, or by leading. You first have to eliminate all the corroded areas and replace with welded-in patches. Some may get away with temporary anything else for a while (perhaps if you leave your car in a air-conditioned room and don't use it), but one needs to make all of the panels sound for road use. Lead-loading is not as easy as one would think, and of concern is the health risk. If you need another reason, try re-welding panels that contain plastic or lead particles from previous repairs, you just can't get a good weld going. Grinding the previous fillers away (the sole means of eliminating them) only makes the metal thinner, thus more difficult to weld well, apart from the obvious weakening. Good Luck, Cheers, Bill in Oz

Location: Euroa,Victoria

Email  
Re: lead loading

Hi Bill

The car in question was NZ assembled and as with most local cars was not painted in hidden areas. Door cappings were perforated after 20 years. Bodge or not, the car has spent another 40 years mostly outside, and cappings OK. It is basically what a professional would have done. Attempting to weld even with MIG would have hugely complicated the exercise.

It is true that, contrary to popular belief, rust will continue under lead if the metal is regularly wet but killed and painted or treated with fishoilene at the back will in many situations last forever.

Location: Auckland, NZ

Email  
Re: lead loading

Bob - Suggest you keep on doing it your way - as long as no-one else does, we'll all be better off. Hopefully the newcomers and the uninitiated will ignore your ideas. Cheers, Bill in Oz

Location: Euroa,Victoria

Email  
Re: lead loading

What an agreeable Antipodean you are Bill.
No philosophical claptrap from you.
We'll hopefully grind the the terminally boring down eventually.

Location: Wessex

Re: lead loading

I once repaired the front wheel arch lips on a Triumph Spitfire using rolled up newspaper held in place with strips of aluminium pop, riveted to the remaining good metal in little depressions made with a ball pain hammer. This was a liberally covered in body filler and sanded to shape. The car was then "resprayed" (given a coat on the bits that show).

This repair was perfectly ok, even in the British weather right up until I sold it, two weeks later!

Location: Teignmouth

Re: lead loading

Hi, I found this on the HAMB (Hokey Ass Message Board) it's in German but a good watch none the less.
http://oldtimer-tv.com/oldtimer/DE/tipps-tricks/index.php?Seite=187

Email  
Re: lead loading

I once attended a car restoring class many years ago, at the stage when the plastic fillers were available but lead loading was still in regular use. The instructor told us that the main reason for using lead in those days was that it was ready for finishing once it was cold, whereas the plastic stuff could not be finished and painted for hours. What was important was to get the job done, get the car out the door, and get the money - nothing to do with how long it would last. I have tried using lead but it needs a knack which I never acquired and I use only the plastic stuff now.

Location: Wellington NZ

Re: lead loading

I did some lead once on my MGB when I restored that. That was 10 years ago and there are a couple of small pics and not much description (sorry) about it here: http://www.asciimation.co.nz/pics/page7.html

Mainly since I wanted to give it a try and also because what I was trying to fix was a badly damaged corner around the rear light fitting. Building up a corner or edge with plastic filler wouldn't have been anywhere near as strong. Lead you can file to give nice, sharp edges.

If you search or ask on forums you'll get lots of reason for both using it and not using it. It's like anything, everyone has an opinion (look at the thread on lock washers as an example).

Some will always emphatically say one way is definitely right and another definitely wrong. I usually ignore those people. Look for the ones who give opinions on both and give a reasoned argument why one way is better in a given situation.

That last bit is important. Lead still has it's place and uses. Given your reason is because you want to try it I say go for it. That's why I did it too.

Trying to remember what I did is tricky, it was a while ago! Definitely get the correct type of body solder and flux. A good panel beating supply place should have it. I did have to hunt about a bit to find it I seem to recall. The local chain type auto places won't have it. I just looked now and found this place in NZ that sell a kit: http://www.restorationautotools.co.nz/auto-body-solder-kit-premium-xidp380520.html I am sure other places have similar available.

You need a good, coarse file. I have one made by Bahco but I can't remember the actual type and don't see it written on it. I can send you a picture of the tooth pattern though. You don't want to power sand lead at all and throw lead dust about.

You also need wooden paddles. Use a hard wood so it doesn't burn as easily. The paddles get coated in tallow to stop the lead sticking to them. I made my own paddles from some scraps of wood I had and they worked fine.

Actually doing the leading is hard to describe. You need a good heat source. I used a Bernzomatic torch with propane (the blue cylinders). Something easy to control as you be wielding the torch in one hand and trying to blob on and smooth the lead with the other.

I started by getting the panel as close to the right shape as possible. My panel beating skills weren't as good back then though! Then get the surface as clean as possible. Wire brush it, remove any rust (I use phosphoric based rust remover) then neutralise that and clean it again.

Then you have to tin the area you will lead. Make sure you tin over the whole area you think you will apply lead. You can't easily go back and tin again later once you've put lead on without ruining what you're already done.

I tinned then wiped the tinning off with a clean, white, cotton rag. You should be left with a nice, shiny surface. Then you can start applying blobs of lead.

Like most soldering/brazing/welding processes it all seems to be a matter of having enough heat in the right places. You need everything in the area you are working close to the right temperature. I find I go wrong when things aren't evenly heated and all of a sudden you hit a cold bit and when trying to put heat into that you mess up what you've already done around it.

The lead will go soft when it is at the right temperature. The descriptions you read say buttery. It's hard to describe without you seeing for yourself but it goes from hard to not totally runny. It doesn't flow exactly but it can be pushed about and moulded with the paddles. But it should be sticking to the tinned areas well. Be prepared, as a beginner, to waste a bit and lose blobs of it onto the floor, especially if you are doing vertical surfaces.

Then it is a matter of juggling the heat while blobbing on bits of almost runny solder and pushing the lead about to where it needs to be. Do't try to smooth it out too much. It is easier to put more on then file it down to where you want. And try to do it all in one go. Once it has cooled trying to go back and add more lead later didn't seem to work very well although that could be down to my lack of experience.

What else? Obviously doing things horizontally rather than vertically is much easier so you don't have gravity working against you. Be aware that putting heat into metal panels might cause them to warp. As i was working on a curved corner that didn't seem a problem for me. Safety - don't power sand the lead, don't breath in the dust, wash your hands well, be careful of the acid flux, don't eat the lead, etc, etc.

I just did it because I wanted to try it and it was a good place to use it in my case. I don't know that I did it right. I am sure I did some things an expert could correct me on. But at least I tried it myself. Whether that makes my advice better than someone who has never done it themselves, has lots of reasons why THEY wouldn't do it and tells you not to bother yourself is up to you :)

I say for the sake of learning give it a go!

The stuff I did 10 years ago is still holding up perfectly on my MGB by the way. I would definitely use it again in a similar situation or if I wanted to seal over a seam somewhere.

Simon

Location: Wellington

Email  
Re: lead loading

If you fancy trying it have go. Struggling with new techniques is all part of the fun. I've never tried lead loading but I've spent endless hours on steaming ash with very mixed results, fascinating and tricky.